Composition | ISOCYANATE PX 5210 | POLYOLPX 5212 | MIXING | ||
Kusanganisa reshiyo nehuremu | 100 | 50 | |||
Aspect | mvura | mvura | Liquid | ||
Color | pachena | bluish | pachena | ||
Viscosity pa25°C (mPa.s) | Nhoroondo ye BROOKFIELD LVT | 200 | 800 | 500 | |
Density pa25°C | (g/cm3) | ISO 1675 : 1985ISO 2781 : 1996 | 1,07- | 1,05 | 1,06 |
Density yechigadzirwa chekurapa pa23°C | |||||
Hupenyu hwehari pa25°C pa150g (min) | Gel Timer TECAM | 8 |
Processing Conditions
Iyo PX 5212 inofanirwa kungoshandiswa mumushini wekukanda vacuum uye kukandwa mune pre-inopisa silicone mold.Kuremekedza kwe70 ° C tembiricha ye mold kwakakosha.
Vacuum casting muchina kushandiswa:
• Pisa zvikamu zvose pa 20 / 25 ° C kuitira kuchengetedza pane imwe tembiricha yakaderera.
• Kuyera isocyanate mumukombe wepamusoro (usakanganwa kubvumira kusara kwekapu tsvina).
Kuyera polyol mukapu yepasi (kapu yekusanganisa).
• Mushure mekubvisa gassing kwemaminitsi gumi pasi pevacuum dururira isocyanate mu polyol uye sanganisa kwemaminitsi mana.
• Kanda musilicone mold, yaimbodziiswa pa70°C.
• Isa muovheni pa70°C.
1 awa ye3 mm ukobvu
Vhura mold, kutonhora chikamu nemhepo yakamanikidzwa.
Bvisa chikamu.
Mushure mekurapa kurapwa kunodiwa kuti uwane zvivakwa zvekupedzisira (mushure mekudzikiswa) 2h pa70°C + 3h pa80°C+ 2h pa100°C.
Shandisa chigadziriso chekubata chikamu panguva yekurapa kwemashure kurapwa
CHERECHEDZA: Elastic memory zvinhu zvinobvisa chero deformation yakaonekwa panguva yekudhirowa.
Izvo zvakakosha kukanda iyo PX 5212 mune nyowani mold pasina kukanda resin kare mukati.
Kuoma | ISO 868: 2003 | Shore D1 | 85 |
Tensile modulus ye elasticity | ISO 527: 1993 | MPa | 2,400 |
Kusimba simba | ISO 527: 1993 | MPa | 66 |
Elongation panguva yekuzorora mukushushikana | ISO 527: 1993 | % | 7.5 |
Flexural modulus ye elasticity | ISO 178: 2001 | MPa | 2,400 |
Flexural simba | ISO 178: 2001 | MPa | 110 |
Choc kukanganisa simba (CHARPY) | ISO 179/1eU : 1994 | kJ/m2 | 48 |
Tembiricha yegirazi (Tg) | ISO 11359-2 : 1999 | °C | 95 |
Refractive index | LNE | - | 1,511 |
Coefficient og light transmission | LNE | % | 89 |
Heat deflection tembiricha | ISO 75: 2004 | °C | 85 |
Maximal kukanda ukobvu | - | mm | 10 |
Nguva isati yademorwa pa70°C (3mm) | - | min | 60 |
Linear shrinkage | - | mm/m | 7 |
Storage Conditions
Upenyu hwesherufu yezvikamu zvese zviri zviviri mwedzi gumi nemiviri munzvimbo yakaoma uye mumidziyo yavo yepakutanga isina kuvhurwa patembiricha iri pakati pe10 ne20°C.Dzivisa kuchengetedza kwenguva yakareba pane tembiricha inodarika 25°C.
Chero gaba rakavhurika rinofanira kuvharwa zvakasimba pasi penitrogen yakaoma.
Kubata Chengetedzo
Hwakajairwa hutano uye kuchengetedza kunofanirwa kucherechedzwa kana uchibata izvi zvigadzirwa:
Iva nechokwadi chekufema zvakanaka
Pfeka magirovhosi, magirazi ekuchengetedza uye zvipfeko zvisingapindi mvura
Kuti uwane rumwe ruzivo, ndapota tarisa kune chigadzirwa chekuchengetedza data sheet.