Iska caabbinta heerkulka sare
Deganaansho cabbir heersare ah
Xoogga sare iyo saxnaanta
Codsiyada ku habboon
Prototypes waxay u baahan yihiin iska caabin heerkul sare leh
Caaryada degdega ah
Xaashida Xogta Farsamada
Guryaha dareeraha ah | Guryaha indhaha | |||
Muuqashada | Semi-translucent | Dp | 13.5 mJ/cm2 | [soo bandhigid xasaasi ah] |
Viscosity | 340 cps@30℃ | Ec | 0.115 mm | [jiirada daawaynta-dhererka vs. In (E) qalooca] |
Cufnaanta | 1.14 g/cm3 | Dhumucda lakabka dhismaha | 0.08-0.12 mm |
Guryaha makaanikada | UV ka dib daaweynta | |||
Walxaha tijaabi | Hababka Imtixaanka | Qiimaha tirada | Hababka Imtixaanka | Qiimaha tirada |
Xoogga Jilicsan | ASTMD 638 | 65MPa | GB/T1040.1-2006 | 71MPa |
Dheeraynta xilliga nasashada | ASTMD 638 | 3-5% | GB/T1040.1-2006 | 3-5% |
Xoog laabashada | ASTMD 790 | 110MPa | GB/ T9341-2008 | 115MPa |
Hababka dabacsanaanta | ASTMD 790 | 2720MPa | GB/ T9341-2008 | 2850MPa |
Izod wuxuu arkay xoogga saamaynta | ASTMD 256 | 20J/m | GB/T1843-2008 | 25J/m |
adkaanta xeebta | ASTMD 2240 | 87D | GB/T2411-2008 | 87D |
heerkulka kala guurka galaas | DMA, tan θ ugu sarreysa | 135 ℃ | ||
Isku xidhka balaadhinta kulaylka (25-50 ℃) | ASTME831-05 | 50 µ m/m℃ | GB/T1036-89 | 50 µ m/m℃ |
Isku xidhka balaadhinta kulaylka (50-100 ℃) | ASTME831-05 | 150 µ m/m℃ | GB/T1036-89 | 160 µ m/m℃ |
Heerkulka lagu taliyay ee farsamaynta iyo kaydinta xabagta sare waa inuu ahaado 18 ℃-25 ℃.